摘要:
This invention relates to an AE series heat resistant compression casting magnesium alloy containing cerium and lanthanum and the composition ingredients and the weight percentage thereof are as follows: Al: 3%˜5%, Ce: 0.4%˜2.6%, La: 0.4%˜2.6%, Mn: 0.2%˜0.6%, and the remainder is magnesium. The raw material of cerium lanthanum mixture of rare earth used is the residual, cheap and overstocked cerium lanthanum mixture of rare earth obtained from common cerium rich mixture of rare earth after the Nd, Rr with high value and good market have been separated. The mechanical performance of this invention at room temperature and high temperature excels that of AE 44 and AZ 91 alloys, and the minimum creep rate of 1.82×10-9 S-1 and the creep percentage elongation in 100 h of 0.17% at the condition of 200° C. and 70 MPa excel these of AE 44 alloy.
摘要:
A high-strength, high-toughness, weldable and deformable rare earth magnesium alloy comprised of 0.7˜1.7% of Ym, 5.5˜6.4% of Zn, 0.45˜0.8% of Zr, 0.02% or less of the total amount of impurity elements of Si, Fe, Cu and Ni, and the remainder of Mg, based on the total weight of the alloy. During smelting, Y, Ho, Er, Gd and Zr are added in a manner of Mg—Y-rich, Mg—Zr intermediate alloys into a magnesium melt; Zn is added in a manner of pure Zn, and at 690˜720° C., a round bar was cast by a semi-continuous casting or a water cooled mould, then an extrusion molding was performed at 380˜410° C. after cutting. Before the extrusion, the alloy is treated by the solid-solution treatment at 480˜510° C. for 2˜3 hours, however, the alloy can also be extrusion molded directly without the solid-solution treatment. After the extrusion molding, this alloy has a strength of 340 MPa or more and a percentage elongation of 14% or more at room temperature and is a high-strength, high-toughness, weldable and deformable rare earth magnesium alloy.
摘要:
A high-strength, high-toughness, weldable and deformable rare earth magnesium alloy comprised of 0.7˜1.7% of Ym, 5.5˜6.4% of Zn, 0.45˜0.8% of Zr, 0.02% or less of the total amount of impurity elements of Si, Fe, Cu and Ni, and the remainder of Mg, based on the total weight of the alloy. During smelting, Y, Ho, Er, Gd and Zr are added in a manner of Mg—Y-rich, Mg—Zr intermediate alloys into a magnesium melt; Zn is added in a manner of pure Zn, and at 690˜720° C., a round bar was cast by a semi-continuous casting or a water cooled mould, then an extrusion molding was performed at 380˜410° C. after cutting. Before the extrusion, the alloy is treated by the solid-solution treatment at 480˜510° C. for 2˜3 hours, however, the alloy can also be extrusion molded directly without the solid-solution treatment. After the extrusion molding, this alloy has a strength of 340 MPa or more and a percentage elongation of 14% or more at room temperature and is a high-strength, high-toughness, weldable and deformable rare earth magnesium alloy.
摘要:
Methods for producing a magnesium-rare earth intermediate alloy, which belongs to the technical field of molten salt electrolytic metallurgical technology. In one embodiment, the method comprises subjecting magnesium chloride, lanthanum praseodymium cerium chloride and potassium chloride to an electrolysis, and adding additional lanthanum praseodymium cerium chloride and magnesium chloride during the electrolysis. In the electrolysis process, neither metal magnesium nor rare earth metal is used, only the chlorides of rare earths and magnesium are used and the rare earth ions and the magnesium ions are co-electrodeposited on the cathode, so as to obtain the intermediate alloy having a melting point close to the eutectic temperature of the rare earth and magnesium. The method has various advantages including but not limited to high operability, simple process and equipment, stable quality of product by mass production and easy for commercial scale production.